Clay shrinkage rate: how to measure it and scale your pots
Measure your clay’s shrinkage with a test bar, work out the percentage from wet to fired, and size a piece so it comes out the finished size you planned.
Clay shrinks twice: while it dries and again while it fires. To measure it, press a line of known length into soft clay, measure it again when dry and again after firing, and use the formula (starting length minus new length) divided by starting length times 100. Ceramics measures drying shrinkage against the wet length, which is what this guide uses.
Two shrinkage figures are not simply added together, so compute the total from the wet length and the fired length. Once you have it, you can scale a design so the finished piece comes out at the size you want.
What happens as clay dries and fires
Digitalfire explains that during drying, clay particles draw together as water between them evaporates, and the piece shrinks. During firing the body densifies and shrinks again. More vitreous bodies shrink more in the kiln.
It also notes that more plastic clays have more drying shrinkage and are more likely to crack, and that shrinkage is relative to the body: there is no single correct figure. The same source gives approximate dry-to-fired shrinkage for whitewares of 7 to 8 percent, vitreous porcelains above 10 percent, stonewares about 5 to 6 percent and earthenwares 3 to 4 percent or less. Treat these as ranges for different families of clay, not a figure for your clay.
How to make a shrinkage test bar
- Roll out a slab of the clay you plan to use, about as thick as your normal work.
- Press a ruler into the soft clay and cut or scratch a straight line exactly 10 cm (or 100 mm) long. A longer line gives a more precise answer.
- Write the clay name, the date and the 10 cm length on the bar, or on a tag that goes with it.
- Let the bar dry completely and slowly, flat, so that it does not warp. Measure the line again with a ruler or calipers.
- Bisque fire it with your normal load, measure again, then glaze fire and measure a final time.
- Write each length down immediately, with the cone of each firing.
Use the same tile in the same position in the kiln if you can. Variation between kiln loads and clay batches is normal, so repeat the test when you change clay.
The formulas
| Measure | Formula | Example |
|---|---|---|
| Starting line (wet) | L1 | 10.0 cm |
| After drying | L2 | 9.4 cm |
| After firing | L3 | 8.7 cm |
| Drying shrinkage | (L1 − L2) ÷ L1 × 100 | (10.0 − 9.4) ÷ 10.0 = 6.0 % |
| Dry-to-fired shrinkage | (L2 − L3) ÷ L2 × 100 | (9.4 − 8.7) ÷ 9.4 = 7.4 % |
| Total shrinkage | (L1 − L3) ÷ L1 × 100 | (10.0 − 8.7) ÷ 10.0 = 13.0 % |
The example numbers are for illustration and do not describe any particular clay. Note that 6.0 plus 7.4 is 13.4, not 13.0. The two stages are measured against different starting lengths, so always take the total from the wet and the final length.
How to size a piece before you make it
Divide the finished size you want by one minus the total shrinkage. With 13 percent total shrinkage, the factor is 0.87. A mug that should be 10 cm tall after firing needs to be thrown about 10 ÷ 0.87 = 11.5 cm tall. A lid that must fit a pot should be measured against a fired pot, not the wet one.
- Use the same clay and the same firing cones as the test bar. A different cone changes how much a body shrinks.
- Shrinkage is not always even in every direction. Thrown ware and slabs can differ, so check a representative piece.
- Test again for every new bag or batch of clay, and keep the numbers with the clay name.
- If a lid or a plate must fit, make a test piece at a tolerance you can adjust.
Why shrinkage matters beyond size
Uneven drying makes uneven shrinkage, and that is what cracks pieces. Digitalfire says excessive or uneven shrinkage causes cracks. Slower, even drying and consistent wall thickness help.
A body that shrinks very little at your cone may be underfired. Digitalfire describes fired shrinkage as a comparative indicator of the degree of vitrification, so if the same clay shrinks less at a lower cone, it may be less dense. Pair the shrinkage figure with an absorption test if strength matters.
Where Glazeloom helps, and where it does not
Glazeloom is a private pottery notebook for iPhone and iPad with no account to create. You can create a piece for a test bar, name the clay in its clay field, mark it as a test tile and write the wet, dry, bisque and fired lengths in its notes. Photos can be tagged as greenware, bisque or fired, so the stages stay together on one piece. A firing note records the cone and atmosphere.
Glazeloom does not calculate shrinkage, scale designs or measure clay. Use a calculator or a spreadsheet for the arithmetic, then keep the result with the piece in your notebook, and search by clay name when you start the next batch.
Related guides
Frequently asked questions
What is a normal shrinkage rate for pottery clay?
It varies with the clay. Digitalfire gives approximate dry-to-fired figures of about 5 to 6 percent for stonewares and 3 to 4 percent or less for earthenwares, and drying shrinkage adds to that. Measure your own clay.
How do I calculate clay shrinkage?
Subtract the new length from the starting length, divide by the starting length and multiply by 100. For total shrinkage, use the wet length and the fired length.
Why are the drying and firing percentages not additive?
Each is measured against a different starting length, so the total is always calculated from the wet length.
Does shrinkage change between cone 5 and cone 6?
It can. Fired shrinkage generally increases as a body matures with temperature, so test at the cone you will use.
Sources and product details
Keep the next result useful
Glazeloom keeps the choices and observations for each piece together. Download the app to explore its notebook.