Crawling, pinholing and blistering all start in the kiln, not in the glaze bucket alone. Crawling is molten glaze pulling into islands that leave bare clay. Pinholes are tiny holes that usually go down to the body. Blisters are larger bubbles that burst and leave rough craters.
Pinholes and blisters are mostly gas escaping from the clay or the glaze while the glaze is molten, and thick glaze, fast firing and stiff glaze melts make them worse. Crawling is mostly about what the glaze was stuck to while it was still dry, and how much it shrank when it dried and melted. The fastest route to a cause is to compare what changed between a good firing and a bad one.
Which fault do you have?
| Fault | What you see | Usual direction of the cause |
|---|---|---|
| Crawling | Glaze has drawn into beads or islands, with bare clay between them | The glaze did not hold on to the surface: dust, cracks in the dry glaze, or too much glaze |
| Pinholing | Tiny holes in the surface, often reaching the clay | Gas rising through the melt from the body or the glaze, and a melt too stiff to close again |
| Blistering | Larger bubbles or craters where blisters burst | Gas from the glaze or body, often with thick glaze or overfiring |
Digitalfire notes that blisters, dimples and pinholes often occur together, so you may see a mix. Treat the most noticeable one first.
Crawling: what to check
Digitalfire defines crawling as the molten glaze pulling itself into islands, leaving bare patches of body. The problem is usually decided before the kiln is closed, so look at how the glaze was applied.
- Dust or grease on the bisque. Wipe bisque with a damp sponge before glazing and let it dry.
- Glaze applied too thickly. A thick dry layer can crack as it dries, and the cracks open up as the glaze melts.
- Dry glaze that cracked or flaked before firing. Do not fire a layer that has already lifted; scrape it off and reapply.
- Glazing over a layer that is already glazed or very smooth. Layered glazes can behave differently from single ones.
- A glaze that shrinks a lot as it dries, which can pull the layer apart and leave gaps.
Digitalfire’s page shows a factory worker pre-wetting and post-wetting critical areas, such as a lid’s concave surface, while dip glazing to avoid crawling. Change one thing at a time, and look at the dried glaze under a bright lamp before it goes in the kiln.
Pinholing: what to check
According to Digitalfire, pinholing is a glaze defect with tiny holes in the fired surface, and the holes normally go down to the body. Its page gives several causes that you can test in turn.
- Gas-producing particles in the clay body, especially a coarse body bisque fired too low. Digitalfire’s own example had a coarse body bisqued only to cone 06.
- A thick glaze layer. Thicker layers pinhole more than thinner ones.
- Fast firing. Faster schedules give gas less time to escape and the melt less time to heal.
- A glaze chemistry that makes a stiff melt. High alumina or zirconium opacifiers stiffen the glaze and make it less able to close the holes.
- A schedule with no hold or slow cool at the end. Digitalfire says potters are free to use drop-and-hold and slow-cool schedules, which can give a good glaze surface on almost any clay body.
Digitalfire’s own worked example counts four causes on one pinholed cone 6 glaze: a very thick layer, a coarse brown stoneware bisque fired only to cone 06, a zirconium opacifier that stiffens the melt, and a boron-rich glaze that starts melting early. The lesson is that defects usually have several contributors, so write them all down.
Blisters: what to check
Blisters are bubbles in the glaze that rise and sometimes burst, leaving rough craters that can be sharp. Digitalfire groups blisters with pinholes and dimples, and its pinholing page says gas from the body and a thick or stiff glaze make them more likely. These are general rules of thumb rather than a diagnosis, so test them one at a time.
- Apply a thinner layer.
- Check that the glaze is fired to the cone on its label and not above it.
- Bisque the ware properly so that the body has already given off most of its gas.
- Try a hold at peak temperature or a slow cool so the surface can settle.
- Compare two firings, one with the blister and one without, and list every difference in the kiln load.
A comparison method that works
- Find a piece that came out well and a piece that failed with the same glaze.
- Write down the bisque cone, the glaze cone, the schedule and any hold, the number of coats and how thick the layer was.
- Note where the piece sat in the kiln.
- Change one factor, for example the coats, and fire a test tile with the old and new version side by side.
- Photograph each tile close up. Keep the photo with the notes.
Two or three comparisons are usually enough to see whether thickness, bisque or schedule is the main factor.
Where Glazeloom helps, and where it does not
Glazeloom is a private pottery notebook for iPhone and iPad with no account to create. Each piece stores the clay, the glaze layers in order with coats and application, the cone and atmosphere, photos and notes. A firing note records the date, kind (bisque, glaze or other), cone, atmosphere, schedule and the pieces fired together, so you can open the bad firing next to the good one. Pieces can be searched and two compared.
It does not diagnose glaze faults, simulate firings or control a kiln. The notebook’s value is that the bisque cone, schedule and coat count are written down when you need to compare them. For the chemistry behind pinholing and blisters, use a glaze reference or ask the glaze maker.
Related guides
Frequently asked questions
Why is my glaze crawling?
The glaze pulled into islands during melting. Check for dust on the bisque, a layer that was too thick, and dry glaze that cracked or lifted before firing.
What causes pinholes in glaze?
Gas rising from the clay or glaze through a melt that is too stiff to close again. Thick glaze, fast firing and a low bisque are the usual contributors.
Will a slower firing fix blisters?
It can help, because gas has more time to escape and the surface more time to settle. Test it on a tile and compare it with the original.
Can I refire a piece with pinholes?
Sometimes a second firing, or an extra layer, can improve a surface. The result is uncertain, so try it on a test tile first.