Glaze crazing: causes, fixes and what to record
Crazing is a web of fine cracks caused by a glaze that shrinks more than the clay. Learn the causes, what to test first and which notes find the pattern.
Crazing is a network of fine cracks in a fired glaze. It happens when the glaze contracts more than the clay body as the piece cools, so the glaze is pulled tight until it splits. Digitalfire describes it as a mismatch of thermal expansion between body and glaze, and says that most of the time the real fix is to change the glaze’s thermal expansion.
That means crazing is a fit problem between one glaze and one clay, not a flaw in either alone. The quickest way to find the cause is to test the same glaze on a different clay, and a different glaze on the same clay, and to write down what each tile did.
How to tell crazing from other glaze faults
Crazing looks like a fine crackle: thin lines running across the glaze in a web or grid. They are cracks in the glaze layer, not in the clay. Some potters hear a faint ticking as a piece cools or sits on a shelf after the firing, and a crazed surface can catch dirt or tea in the lines.
It can show up the moment the kiln is opened, or later. Do not assume a piece that looked clean on unloading will stay that way, and keep an eye on test tiles for a few weeks before you trust a result.
| Fault | What you see | Direction of the stress |
|---|---|---|
| Crazing | Web of fine cracks across the glaze | Glaze shrinks more than the body and is under tension |
| Shivering | Flakes of glaze lift or peel off, often at edges and rims | Glaze shrinks less than the body and is under compression (the opposite of crazing) |
| Crawling | Glaze pulls into islands and leaves bare clay | Not a fit problem: the glaze did not stay attached while melting |
| Crackle glaze | A deliberate, even crackle pattern | Crazing chosen as decoration |
If your fault looks like bare patches or tiny holes rather than cracks, see our guide to glaze crawling, pinholing and blisters instead.
Why glaze crazes
Every clay body and every glaze expands when heated and contracts when cooled, each by its own amount. When the glaze contracts more, it is stretched and cracks. The most common causes, in the order most worth checking, are listed below.
| Cause | What is going on | What to test |
|---|---|---|
| Glaze expansion too high | Glazes rich in sodium and potassium expand and contract more | Choose a glaze formulated to fit your clay, or have its chemistry adjusted so that high-expansion oxides are replaced by lower-expansion ones |
| Clay body does not match the glaze | The same glaze can fit one body and craze on another | Fire the glaze on two or three clays in the same kiln load |
| Body not fully matured | A clay fired below the temperature it was designed for stays more porous, and a body that is not mature can change how the glaze fits | Check the cone range printed for the clay and compare it with the cone you fired |
| Sudden temperature change | Hot ware moved quickly to cold, or a cold piece filled with hot liquid, stresses the glaze | Warm and cool ware gradually and note whether crazing appeared after use |
| Thick glaze or heavy layering | A thicker layer carries more stress, and combinations behave differently from single glazes | Make a tile with one coat and a tile with the normal number of coats |
Digitalfire adds an important warning: changing glaze thickness, the firing or the cooling can hide a mismatch for a while, but a real expansion mismatch will show itself sooner or later. Treat those changes as ways to learn about the fit, not as the cure.
A test sequence that finds the cause
- Photograph the crazed piece in raking light so the lines show, and write down the clay, the glaze layers in order, the number of coats, the cone and the kiln.
- Make three tiles from the same clay: your normal glaze application, one thinner coat and one thicker coat. Fire them together. If only the thick tile crazes, the fit is marginal and thickness is exposing it.
- Glaze the same glaze on a second clay body in the same firing. If it does not craze there, the body is the difference.
- Fire a different glaze on the original clay. If that one holds up, the first glaze is the problem.
- Wait several weeks and check again. Keep each tile with its notes so you can match the result to the record.
- If the glaze is a commercial product, contact the maker with your clay, cone and firing details. They know the cone and body it was tested on.
Change one thing per tile. If you change the clay, the coats and the cone at once, you will not know which one mattered.
Is crazed pottery safe for food?
Cracks in the glaze let liquid reach the clay underneath, and the lines are harder to clean. For that reason many potters avoid using crazed pieces for food and drink, or keep them for decoration. We do not give safety rulings. If a piece will hold food, ask your studio, the glaze manufacturer or a testing laboratory, and do not rely on a notebook entry to decide.
Can a crazed piece be rescued?
A piece that has already crazed is hard to save, because the fit between that glaze and that clay has not changed. Applying more glaze and refiring is a gamble and usually repeats the result unless something about the pairing changes. The reliable approach is to correct the glaze or the body on the next batch and keep notes so you do not repeat the pairing.
Some potters want crackle on purpose. If so, make it a controlled test: record the glaze, clay and cone that produced a pattern you like, so you can reproduce it.
What to record so the pattern shows up
- Clay body, with the maker’s name and the cone range on its label.
- Every glaze layer in order, and the number of coats.
- The cone and atmosphere of the firing, and the kiln or studio.
- The date the crazing appeared, if it came after the firing.
- A photo of the surface, and a one-line note on how the piece was used or washed.
After a few tiles, a search across your own records usually makes the pattern obvious, for example every piece with one glaze that crazed on one clay and held on another.
Where Glazeloom helps, and where it does not
Glazeloom is a private pottery notebook for iPhone and iPad with no account to create. A piece or glaze test holds the clay, the ordered glaze layers with the number of coats and how each was applied, the cone and atmosphere you enter, photos and notes. A firing note can store the date, cone, atmosphere, schedule and the pieces in the kiln. You can mark a piece as a test tile, search your own history by clay or glaze, and compare two pieces side by side.
Glazeloom does not measure glaze fit, calculate thermal expansion or judge food safety. It keeps the observations in one place so that you can see which pairings crazed. Use glaze chemistry software or your glaze supplier for the expansion maths. Make a backup before changing phones; our back-up guide explains how.
Related guides
Frequently asked questions
What causes crazing in pottery glaze?
The glaze contracts more than the clay body while cooling, so the glaze is stretched and cracks. Digitalfire calls this a mismatch of thermal expansion, with the glaze’s expansion higher than the body’s.
Can crazing appear after the piece has cooled?
Yes. Some pieces craze on unloading and others weeks later, so check test tiles again after a while before you decide a glaze fits.
Does a thicker glaze craze more?
A thicker layer tends to show a marginal fit more readily. Digitalfire cautions that changing thickness or firing can hide a mismatch without removing it, so test on more than one clay.
Is crazing the same as crackle glaze?
Both are cracks in the glaze. Crackle glaze is a crackle pattern chosen on purpose, while crazing is unwanted. The mechanism is the same.
Sources and product details